44. Staining of a tree. 45. Aniline mordants for wood. 46. ​​Turpentine mordant.
47. A mordant for imitation of an oak tree. 48. A mordant for simulating a walnut tree.
49. A mordant for imitation of a rosewood tree. 50. Mildew for mahogany imitation.
51. Mildew for simulating rosewood. 52. Mordant for simulating gray maple.
53. A mordant for imitation of ebony. 54. A mordant for (smoking) wooden pipes.
55. Waxing the tree. 56. Preparation of wax polishes for polishing wooden products.
57. Joinery polishing. 58. Strong drawings on wooden plywood. 59. Bronzing of a tree. 60. Liquid bronze.
61. Cleaning of gilding. 62. Black stains for the horn. 63. Gray mordant for the horn. 64. Red mordant for the horn.
65. Turtles for horns. 66. Aniline mordant for bone. 67. Whitening ivory.
68. Staining billiard balls. 69. Silver polished ivory.
-------------------------------------------------- -------------------------

44. Staining of a tree.

Abroad, the following method of wood staining is widespread, having the advantage over commonly used methods in that, with this method, the wood is impregnated with paints to a considerable depth and can be polished without damaging the applied paint. The method consists in the following. Prepare a batter from rye, wheat or potato flour, smear it on a sheet of paper, cardboard or thin sheet with a thickness of 0.5 mm. On this layer, paint is applied in the form of a powder or in the semi-liquid state in which they are used to make colored paper, after which everything is applied to the object to be painted; On top of paper or cardboard put a holeted sheet and tighten brackets. In this form, all this is immersed in boiling water. Here, the colorants dissolve and impregnate the wood, and the dough solidifies so firmly that it keeps the overlaid colors together, preventing them from merging with each other. Thus, it is possible to paint the tree simultaneously in different colors, not allowing the latter to merge; It is possible to apply veins, patterns, etc. All kinds of colors. The deeper you must penetrate into the wood of the paint, the longer it takes to keep objects in hot water. At the end of the dyeing process, the dough is washed off with water and the painted surface is allowed to dry well in a dark room. Instead of the direct use of dry paints in powder, which are suitable for all kinds of paints used in the dyeing business, another cheaper method can be used, which consists in the fact that the wood sawdust is impregnated with paints beforehand and already applied in the above way to the liquid dough.

45. Aniline mordants for wood.

Recently, aniline inks have gradually replaced all previous vegetable paints due to cheapness and an easy way of using.
I. Yellow mordant.
A) light yellow:
100 g of yellow aniline in 3 l of soft water are dissolved.
B) dark yellow:
100 g of xanthine are dissolved in 2.5 l of water.
C) saffron-yellow:
Dissolve 100 g of safranin in 2 liters of water.
D) lemon yellow:
Dissolved 100 g of naphthalene yellow in 2.5 liters of water.
E) orange-yellow:
Dissolve 100 g of orange aniline in 2.5 liters of soda.
E) red-yellow:
100 g of orange aniline, 20 g of eosin in 2.5 l of water are dissolved.
II. Green mordants.
A) light green:
Dissolve 100 g of methyl herbs in 2 liters of soft water.
B) dark green:
100 g of methyl greens are dissolved,
20 g of blue aniline (alkaline) in 2.5 l of water.
C) yellow-green:
Dissolve 100 g of green (acid) in 2.5 liters of water.
D) herbaceous-green:
100 g of malachite green, 10 g of yellow naphthalene in 2.5 l of water are dissolved.
E) malachite-green:
Dissolve 100 g of malachite green in 2 liters of water.
III. Blue mordant.
A) light blue:
100 g of Bleu de ciel are dissolved in 3 liters of water.
B) dark blue:
Dissolve 100 g of Bengal blue in 2 liters of water.
C) greenish blue:
Dissolve 100 g of Bleu tres vert in 2 liters of water.
IV. Violet mordant.
A) light purple:
100 grams of methyl ether are dissolved in 3 liters of soft water.
B) dark purple:
100 grams of methyl ether are dissolved in 2 liters of water.
C) reddish-violet:
Dissolve 100 g of methyl ether, 20 g of eosin in 3 liters of water.
D) bluish-violet:
Dissolved 100 grams of methyl violet, 20 g Bleu de ciel in 2.5 liters of water.

46. ​​Turpentine mordant.

As you know, when etching a tree, you still use solutions of organic paints in water or alcohol. This method, however, has one significant drawback: the surface of the wood to be stained from alcohol or water becomes rough, so that after etching it has to be smoothed with a glass skin, and with such polishing the paint is obliterated in places and there is a need for a second coating, which entails a new grinding Etc., until you get an impeccably smooth surface. Patented by the company "Yungas" in Württemberg mordant is that instead of alcohol or water, the solvent of the paints is turpentine. With the use of such mordants, the fibers of the wood do not swell at all, what precludes the appearance of roughness, and, consequently, the need for grinding. Depending on the structure of the tree, more thin or coarse, one or two coatings are sufficient to obtain the required shade. Sami solutions for walnut, rosewood, light or dark oak, etc. Are prepared in the usual way with the replacement of water or alcohol with turpentine. So, to get a good mordant under a walnut tree, dissolve 600 g of brown paint and 15 g of orange in 1 liter of turpentine. Then the solution is filtered and a filtered solution of 100 g black ink in 3 liters of turpentine is added to it. If the resulting mordant turns out to be thick or inadequate to the desired tone, it is bred with turpentine.

47. A mordant for imitation of an oak tree.

Cook for an hour a mixture of 0.5 kg of Kassel land, 50 g of potash in 1 liter of rainwater, then the resulting dark broth is filtered through the canvas and cooked until the syrupy state. After that, pour it into completely flat boxes of tin (lids from under the tins), give a hardening and crushed with a pistil into a large powder, which after boiling with water (1 part of the powder in 20 parts of water) for a few minutes gives an excellent mordant For imitation of an oak tree.

48. A mordant for simulating a walnut tree.

Ordinary walnut tree has a light brown color, which even after polishing does not look very nice. Therefore, the natural walnut tree should be given a darker tone, which is achieved by treatment with a solution of potassium permanganate. As soon as the tree dries, this solution is applied for a second time, but only to some places, so that the stiffness is obtained, and they try to make it look natural. The walnut tree, along with the dark veins, is almost black, it is best to simulate such places with black stain (see ebony). The quality of imitation will depend on the art of the worker.

49. A mordant for imitation of a rosewood tree.

Rosewood tree has a dark brown color with characteristic reddish veins. Since the walnut tree is closest to rosewood, then to imitate the latter and take walnut, with other varieties of wood does not produce such a beautiful fake.
The walnut is first ground with pumice stone and then evenly covered with a sponge or cotton wool with the following composition: 3 parts by weight of brown aniline and 100 parts by weight of alcohol. After drying, the operation is repeated if necessary. The dark veins of the rosewood tree appear with the aid of a flat brush adapted for this purpose by the decoction of a kampesheva tree. After drying, the tree is wiped with a sponge impregnated with a weak solution of potassium dichromate, then a small amount of oil is rubbed into it and finally polished. For polishing use a solution of red shellac in alcohol to which is added so much alcohol solution of the orseli, so that the red color inherent in this polish, had the proper strength. Then, the reddish veins and the dark-brown color of the rosewood tree are obtained from the joint action of the coloring substances contained in the wood and the polish, while other places take a reddish-brown color, which is also observed in the rosewood tree. Depending on the amount of solution taken, the Orsley produces a lighter or darker color of the rosewood tree.

50. Mildew for mahogany imitation.

The wood intended for the mordant must be well dried, and the application of the mordant is best done with a brush, which after each use must be washed and dried immediately.
1) A very beautiful and strong mordant is prepared by mixing in the bottle 500 g finely chopped sandalwood, 30 g potash and 1.5 liters of water. The mixture is left to stand in a warm place for a week, often shaking. Then the liquid is filtered through cloth and stored in a suitable container before use. In another bottle, dissolve 30 grams of alum when heated in 1.5 liters of water, filter and store. The object to be etched is treated with the heated first solution several times until the desired color is obtained, after which it is coated with a second, also heated, liquid. Mix both fluids in one should not. After drying, the etched object is wiped with a cloth with linseed oil.
2) Recently, sandalwood is often replaced with aniline paints, soluble in water. The advantage of aniline paints is their large coating ability. To paint a mahogany, the paint "Ponceau" is very suitable. In 3 liters of water, dissolve 100 g of aniline "Ponce". This solution is applied to the staining tree once or twice, depending on the color that they want to receive.

51. Mildew for simulating rosewood.
The pink tree is characterized by dark red veins. To simulate this tree, maple is taken, as the most suitable in its structure. Maple boards or plywood should be carefully ground before going into processing, as only in this case they are well stained.
1) To simulate a pink tree, two colors are prepared: one for obtaining lighter red veins, and the other for darker ones. These paints are solutions of aniline in 60% alcohol. Paints are made according to the following recipes.
1) Light red: 1 part by weight of coralline, 1 part by weight of rosée, 100 parts by weight of alcohol or vodka.
2) Crimson: 1 part by weight of coralline, 1 part by weight of rosine, 0.1-0.2 parts by weight of brown aniline, 100 parts by weight of alcohol or vodka.
Using a brush divided into several parts, paint the No1 vein with paint so that between each two there is a space of 10-12 mm. As soon as these veins dry out, some of them intensify here and there with the same paint. After this, the veins are painted with thin column brushes in such a way that they do not seem sharply outlined. Finally, paint the No2 paint the darkest veins. The whole drawing must be executed so that the natural veins of maple pass between the veins.
If a maple tree came from dark varieties, then for clarification, immerse it in a solution of 1 part of bleach in 20 parts of water and, after the tree is submerged, add 1 liter of strong vinegar to the solution, causing the tree to lighten in half an hour. Then it is placed for a day in a solution of 1 part of soda in 10 parts of water, taking out of which they wash and dry. A tree treated in this way can be painted with the most gentle tones penetrating deep into the tree.
2) For a rougher imitation of a rosewood, without painting veins, you can use the following mordant. For this, two liquids are prepared: 100 g of sandalwood is dissolved by boiling in 300 g of water; 100 g of Kassil land and 10 g of potash are dissolved in 300 g of water. Then mix the two liquids together, filter and pour into different tins.

52. A mordant for imitating gray maple.

As a gray mordant for wood, it is good to use a water-soluble strong and light aniline dye nigrosine. A solution of 7 parts of nigrosine in 1000 parts of water stains the tree in a beautiful silvery-gray color, which is so strong that even after two years it does not change at all.

53. A mordant for imitation of ebony.

Smoothly trimmed black (ebony) wood has a pure black color without gloss and has such a fine structure of fibers that the latter can not be seen with the naked eye. The specific weight of this tree is very large. Polished ebony so well that the polished surface of it is a kind of a black mirror. In order to achieve a good imitation, you should take a solid, solid wood with a gentle structure. This condition is met, for example, beech and pear tree.
1) Items with carefully ironed surfaces are etched with sulfuric acid, after which they are washed with water and dried. After treatment with this acid, the objects are etched with a solution of kampeshevogo wood or iron mordant.
In the first case, after preparing a 10% solution of Kampesheva wood in water, they cover the objects, allow them to then dry and then treat them with a 1% solution of potassium dichromate in water.
In the second case, use an iron mordant, which is prepared as follows: the old iron is processed for a few weeks with strong vinegar, taking 10 parts of vinegar per 1 part by weight of iron. Then boil 1 part by weight of ink nuts with 10 parts by weight of water. The object to be stained is placed for a few days in the resulting solution of acetic acid iron, 1st solution), then it is dried in air, and then placed also for several days in the decoction of the ink nuts. If the object in its size is inconvenient to immerse in a liquid, then it is treated with a brush several times with decoction of the ink nuts until a dark yellow color is obtained and then covered with a solution of acetic acid iron or ferrous sulfate solution until a black color is obtained. Both in that, and in another case, the operation is conducted until the color of the desired density is obtained. It is even better to cover the object alternately with an infusion of ink nuts, then an infusion of acetic acid iron or iron vitriol, each time it is necessary to dry the surface of the object and then cover it again.
2) Extremely beautiful black coloring of the tree can be achieved by treating it with black aniline paint nigrosine, which dissolves in water. For this purpose, dissolve 8 parts by weight of nigrosine in 10 parts of water and cover the object with this solution. After drying, a solution of copper in hydrochloric acid, which is prepared from 20 parts by weight of hydrochloric acid and 1 part by weight of copper, is applied to it. Immediately after applying a solution of copper chloride, the tree takes on a beautiful matte black color, very similar to the color of a real black (ebony) tree. Polishing gives it a strong shine.

54. Mordant for wooden (smoking) pipes.

A good mordant, which gives extremely beautiful shades on the wooden heads of the tubes, is prepared by grinding in the water of equal parts of potassium dichloride (hrompic) and oxalic acid. When the release of gases from the liquid stops, the mordant is ready. It can be stored for a long time in a well-sealed flask. The harder the solution, the darker the color the tree gets. If one dive or coating is not enough to achieve the desired color, the operation should be repeated. This same mordant can be used for other similar wooden products.

55. Waxing the tree.

There is the following simple method, quite suitable for preparing wax for waxing expensive wooden furniture. Take 100 g of good yellow wax, finely chop it and add 12 g of mastic or 25 g powdered rosin. These substances are piled in an earthen vessel and dissolved on coal. When the whole mass melts, it is removed from the fire and immediately topped with 50 g of warm turpentine. All are thoroughly stirred and poured into a tin or stone jar. In this form, the composition is stored before use. To polish furniture take a small amount of composition on a piece of woolen cloth and rub the tree, which quickly acquires a very beautiful and soft shine. Waxed furniture thus very long retains a beautiful polish.

56. Preparation of wax polishes for polishing wooden products.

Of the many compositions, the following can be considered the best:
1) 25 parts by weight of finely planed stearin are added to 12.5 parts of turpentine and the mixture is heated until the stearin is completely dissolved.
2) Dissolve 25 parts of wax in an glazed pot and then, when the wax is dissolved, the vessel is removed from the fire and 40 parts of turpentine are added to the wax.
3) Heating 10 parts of the kopalovy lacquer, add to it 40 parts of wax and, when the latter dissolve, add, gradually stirring, 75 parts of turpentine.
4) 30 parts of wax and 1.5 parts of rosin are dissolved on fire, then, removing the vessel from the fire, add 14.5 parts of turpentine.
5) Pour 2.5 parts of potash into 30 parts of water and boil, then add 5 parts of finely stratified wax and heat the whole mixture until a homogeneous soap mass is obtained.

57. Joinery polishing.

Политура подбирается по оттенку соответственно цвету полируемого дерева, от красновато-коричневого до белого цвета или, вернее, бесцветного. Желательный оттенок получается, если брать в разных пропорциях две основные политуры.
1) Красно-коричневая политура: 1 часть красного шеллака, 4 части спирта.
2) Белая политура: 1 часть выбеленного шеллака, 5 частей спирта.
Выбеленный шеллак готовится из обыкновенного следующим образом: 4 весовых части шеллака смешивают с 1 частью соды и растворяют при размешивании в 15 частях воды до полного растворения смолы, т.е. пока жидкость не станет вполне прозрачной. Затем дают отстояться и сливают прозрачный раствор без осадка в другую посуду. Здесь к прозрачному раствору добавляют раствор 4 весовых частей хлорной извести в 4 весовых частях воды и оставляют смесь в покое на два дня. После этого вливают в смесь понемногу соляную кислоту, пока не перестанет выделяться осадок смолы. Затем остается лишь хорошо промыть осадок смолы водой, чтобы удалить следы соляной кислоты, и высушить.

58. Прочные рисунки на деревянных фанерах.

Предварительно готовят раствор из 10 весовых частей медного купороса, 6 частей голландской сажи и 3 частей спирта. Затем на лицевой стороне фанеры набрасывают синим карандашом легкий контур рисунка, после чего все пространство, обведенное синим карандашом, покрывают тонким контуром с помощью стального пера, обмакиваемого в вышеуказанный раствор, глубоко проникающий в ткань дерева. Когда весь рисунок высохнет, фанеру помещают под кран с водой таким образом, чтобы она в течение 20 часов промывалась непрерывно равномерными и слабыми струйками свежей воды. При такой обработке рисунок на фанере так глубоко проникает в дерево, что контуры его ясно обозначаются на противоположной стороне фанеры, и, сколько бы последняя затем не подвергалась обработке, рисунок не сотрется.

59. Бронзирование дерева.

Разведенным раствором жидкого стекла равномерно обмазывают при помощи кисти предметы из дерева, а затем их обсыпают золотой бронзой из баночки, горлышко которой обвязано кисеей. Бронза после высушивания так сильно пристает к предмету, что поверхность его даже можно отполировать агатом. Способ этот рекомендуется для бронзирования рам к картинам и для других предметов.

60. Жидкая бронза.

Жидкая бронза, не дающая на предметах зеленой окраски от образования ярь-медянки, получается при нейтрализации кислот, содержащихся в даммаровой смоле. Для этого поступают следующим образом: 250 г мелко растертой даммаровой смолы растворяют при частом взбалтывании в 1000 частях бензина. Затем доливают 250 г 10%-ного водного раствора едкого натрия, взбалтывают в течение 10. минут и оставляют стоять. Скоро образуются два слоя: верхний, содержащий раствор смолы в бензине, нижний - водный раствор солей натрия со смоляными кислотами. Первый из них сливают, смешивают с новой порцией 10%-ного раствора едкого натрия, взбалтывают и дают отстояться. Этот верхний слой, содержащий смолу, совершенно свободен от кислот. К такому раствору можно добавить 1/4 л часть золотистой бронзы, не боясь образования ярь-медянки.

61. Чистка позолоты.

Чистка позолоты, в особенности на дереве, требует весьма осторожного обращения. Предварительно с позолоты должна быть сметена вся пыль, затем позолоту осторожно вытирают мягкой губкой, еще лучше кусочком ваты, слегка смоченной винным спиртом или скипидаром. Вместо названных жидкостей употребляются также хорошее крепкое пиво, раствор так называемого марсельского мыла или смесь из 10 частей нашатырного спирта и 40 частей мыльного спирта.Хорошим средством для чистки позолоты считаются также яичные белки, которыми осторожно вытирается предмет при помощи кусочка фланели. Можно употреблять смесь белков (2-3 яйца) с 18 г жавелевой воды; этой жидкой смесью с помощью мягкой кисточки вытирают слегка позолоту, особенно наиболее потускневшие места. Наконец, той же цели может служить чистый винный уксус, которым покрывают позолоту посредством мягкой щетки, губки или кусочка паты. Спустя 5 минут уксус осторожно смывают чистой водой, не вытирая ничем.
Для чистки золоченной бронзы помимо нашатырного спирта, разбавленного водой, хорошие результаты дает еще следующий способ: позолоту вытирают прежде всего щеткой, смоченной водой. Затем покрывают с помощью мягкой кисти смесью, составленной из 60 частей воды, 15 частей азотной кислоты и 2 частей квасцов, после чего жидкости дают высохнуть, не вытирая ее.

62. Черные протравы для рога.

Как известно, роговые изделия, как-то гребни, пуговицы, запонки и т.п., часто окрашиваются в черный цвет для подделки их под более дорогие сорта. Для этого существует несколько способов:
а) Изделия из рога вымачиваются в следующем растворе, который готовится на холоде: 8 частей ртути растворяются в 8 частях концентрированной азотной кислоты и 32 частях мягкой воды. В этой протраве изделия оставляют на всю ночь, после чего их вынимают и промывают водой до тех пор, пока промывная вода не будет более обладать кислой реакцией. От такой обработки гребни окрашиваются в красный цвет, а в случае употребления более концентрированного раствора ртути - в коричневый. После этого гребни переносятся в слабый раствор серной печени (1 г на 1 л воды) на 1-2 часа. Окрасившиеся теперь в черный цвет гребни промываются сначала чистой водой, затем подкисленной уксусом и, наконец, чистой водой. После этого их высушивают и полируют. С помощью такой обработки получаются роговые изделия, не уступающие, по мнению знатоков, изделиям из рога буйвола. Полировка окрашенных предметов должна производиться осторожно, так как протрава не проникает в рог достаточно глубоко.
б) Роговые изделия кладут на ночь в холодный водный раствор азотнокислой окиси свинца (в отношении 1:4), после чего их помещают на полчаса в 3%-ный раствор соляной кислоты и, наконец, промывают водой. Если окраска получится неравномерной, то операцию повторяют еще раз. Эта прекрасная протрава значительно поднимает ценность роговых изделий.

63. Серая протрава для рога.

Для окраски рога в серый цвет проварить его сначала в течение 15-30 минут в насыщенном растворе свинцового сахара, затем промыть его в чистой воде и положить на 20-25 минут в нагретый до 60|С раствор азотнокислой, закиси ртути. Этот способ непригоден для гребней, так как зубья страдают от варки.

64. Красная протрава для рога.

Для окраски рога в красный цвет рекомендуется следующий способ. Светлый рог варят 30 минут в растворе, состоящем из 20 г сафлора и 10 г соды в 0,5 л воды, и после этого кладут на полчаса в слабый раствор виннокаменной кислоты. Затем вынимают и, обмыв, опять кладут в сафлоровый раствор и потом опять в раствор виннокаменной кислоты и так продолжают до образования желаемого цвета. Таким образом легко получить все оттенки от самого светлого до темно-красного цвета. Необходимо только помнить, что виннокаменная ванна всегда должна быть последней.

65. Черепаховые протравы для рога.

Если хотят придать роговым изделиям черепаховую окраску, то применяют следующий способ. Роговые изделия обрабатываются сначала разбавленной азотной кислотой (1 часть на 3 части воды) при температуре 30-35|С и затем протравляются смесью из 2 частей соды, 1 части свежеобожженной извести и 1 части свинцового глета. Действие протравы должно продолжаться не более 10-15 минут, чтобы пятна на роге получились желто-коричневыми. После этого, смыв с рога протраву, вытирают его тряпочкой и кладут в холодную красильную ванну, состоящую из 4 частей отвара красного дерева (в 10| по Боме) и 1 части раствора едкого натрия (в 20| по Боме). Затем рог вынимают из ванны, тщательно промывают водой и полируют по прошествии 12-16 часов. Красильный отвар готовится вывариванием 0,5 кг фернамбукового дерева в 4-6 литрах воды. Если добавить к протраве оловянные соли, то получится ярко-красный оттенок.

66. Анилиновые протравы для кости.

Травление кости анилиновыми красками проще, чем другими способами, так как оно проводится в холодной ванне, чем устраняется возможность растрескивания предметов. Травление производится следующим образом: предметы кладут в таз и наливают столько воды, чтобы они были полностью покрыты ею. Затем к жидкости добавляют 2 чайные ложки уксуса и около 1 г краски, причем все равно, растворима ли последняя в спирту или воде. Для нужных оттенков выбирают подходящие анилиновые краски или составляют их из нескольких. Костяные предметы оставляют в жидкости на 4-8 часов и вынимают тотчас же по достижении желаемой густоты тона. Затем их обмывают водой, высушивают и полируют венской известью с мылом. Спиртовые лаки и политуры здесь нельзя употреблять, так как они могут растворить краску на поверхности кости.
Если нужно окрасить бильярдный шар из слоновой кости в два цвета параллельными полосами, то его уже отшлифованным зажимают между тремя тонкими палочками, вставленными вертикально в небольшую дощечку, покрывают среднюю полосу масляным лаком и окрашивают сперва один сегмент, погружая им шар вместе с дощечкой в соответствующую анилиновую протраву. Окончив окраску, дают ей просохнуть, а лак счищают скипидаром и окрашивают эту часть в требуемый цвет, предварительно закрыв масляным лаком уже готовую часть шара. Подобным же образом поступают, если шар надо окрасить с трех или четырех сторон.

67. Беление слоновой кости.

Чтобы вернуть пожелтевшей слоновой кости первоначальную белизну, практикуют один из следующих способов. Слоновая кость покрывается тонким слоем скипидара и выставляется дня на 3 или 4 на солнце. Другой способ: слоновую кость погружают на некоторое время в перекись водорода, после чего ее насухо вытирают. Чтобы ускорить процесс беления, кость подвергают действию лучей синей кварцевой электрической лампы. При том и другом способе кость становится совершенно белой.

68. Окрашивание бильярдных шаров.

Чтобы окрасить бильярдные шары в красный цвет, их следует погрузить в уксус, в котором предварительно размачивается кошениль, и прокипятить в этом уксусе в течение нескольких минут. Затем, для придания цвету более густого оттенка, шары переносятся на 10-15 секунд в очень слабый раствор поташа. Продержав бильярдные шары 6-8 часов в уксусе или растворе квасцов, их легко затем окрасить в отличный желтый цвет, для чего достаточно опустить на некоторое время в квасцовый отвар шафрана. Окрашивание в зеленый цвет достигается погружением шаров в уксус, в котором растворена 1часть нашатыря на 3 части медянки. Если затем перенести эти шары в горячий щелок из поташа, то они окрасятся в голубой цвет. Наконец, чтобы окрасить бильярдные шары в черный цвет, их следует подержать несколько минут в горячем отваре кампешевого дерева (синего сандала), а затем перенести в раствор уксуснокислой соли.

69. Серебряная полировка слоновой кости.

Изделиям из слоновой кости можно придать очень эффектную блестящую серебряную полировку. Вот очень простой способ: по окончании отделки изделие из слоновой кости погружается в слабый раствор азотнокислого серебра и, как только оно окрасится в темно-желтый цвет, его погружают в чистую воду и выставляют на солнце. Через каких-нибудь три часа кость полностью чернеет; тогда ее тщательно натирают сыромятной кожей, после чего кость приобретает красивую блестящую серебряную полировку.