TECHNOLOGY OF MANUFACTURING OF CONDUCTIVE ADHESIVE GLUE

Glossary of terms

But | B | In | | G | D | Ж-и | To | | L | M | N | About | N | Rs | T-y | Fc | Ш-я

Recipe N1:

Graffiti powder (the most refined tortured) ............. 15g.
Separately powdered ................................................ .................. 30d .
Copolymer vinyl chloride-vinyl acetate .................................... 30d .
Acetone is neat ................................................ ............................. 32d.

In the facade stupa, all components are thoroughly mixed. The finished glue (silky-colored liquid of gray-black color) is transferred to a glass container with a printer.

Before using the adhesive, stir well with a glass rod. The viscosity of the adhesive can be reduced by adding acetone. It dries for 10-15 minutes. This recipe is used if you need a RELIABLE connection with sufficient electrical conductivity.

Recipe N2:

Separate powder .......................................... 60g
Graffiti powder ........................................... 6 g
These substances are well mixed in mortar. The binder is added to the resulting mixture:
Nitrocellulose ................................................. .. 4 g
Acetone or ethyl acetate .............................. 30g
Natural rosin .......................................... 2.5 g

All substances are thoroughly mixed and well rastirayut until obtaining a homogeneous paste mass. Before using the adhesive again, small quantities of acetone or ethyl acetate are added, until the desired viscosity is reached.

It can be similar to use the other binder:

Shellac natural ......................................... 3g
Ethyl alcohol denatured ............. 31g

This binder is poured into the powdered hodgepodge of grain as well as graffiti.

Glue with shellac binding agent is used for gluing mechanically unloaded elements.